mae

Hello everyone,

I'm quite new to the cyanotype process. But I spent quite some time in dark rooms developing film and creating silver prints.

After buying a cyanotype kit, I started testing with different negatives, exposures etc.

My latest test print, with which I hoped to figure out the right timing for the exposure, shows some brush streaks in an area that should be purely white.

The paper (Hahnemühle Platinum Rag) was coated 2 weeks prior to the exposure with normal room lighting (warm white led bulb) and was then dried in a fairly dark room before storing it between two pages of a heavy book 🙂

The exposure happened in the sun with a negative on top giving coverage values from 0% to 100% in the horizontal direction.
I used a thik cardboard stepping downwards every 30 seconds.
PXL_20221013_101648889.jpg
Any idea why I don't get a clear white in the lower right corner? Might it have been exposed already while brushing the solution on?
I had some prints where I got a cleaner white and others where this phenomenon also showed as seen here.

Watching some YouTube videos, I also realized that some users have almost yellow solutions A and B where my B solution is almost black.

PXL_20221013_102000138.jpg

I thought it's not too hard to fill a bottle with distilled water 🙂 Is this normal? Or might the chemistry be the problem?

I'm glad for any suggestions

Thank you in advance and Happy printing
mae

Reply 0 0
Jacquardmod Jacquardmod
I had another customer with this same issue.  She was able to solve it by reducing the amount of solution B.  She went from 1:1 to 2:1 and got less grainy results.  Solution B should be more yellow, but this is just not a fully reduced chemical.  It can still make good prints.  I believe that extra oxidized material is hampering you somewhat.  Can you let me know what the batch numbers on the bottles are especially part B?  

Is it batch 102210?


try reducing part B to 2:1 or even 1.5:1 and see if that helps.  If not, send me an email at techsupport@jacquardproducts.com and we can get you a better batch.  
Reply 0 0
mae

Thank you for your reply. I will coat the next papers with a 2:1 mix and see where I get with that.

The batch of solution B is 103549

I remember when adding the water and agitating, that one of the bottles got a bit cold. I thought that this endothermic reaction is the natural process, but it might be a further hint for you?

 

Reply 0 0
Jacquardmod Jacquardmod
Thanks for the batch.  
Reply 0 0
mae
Hey there,

Today I was able to recreate the situation/outcome and also to fix the issue.

I made two prints. The first on a paper I coated two weeks ago. (Hahnemühle again coated when the paper was damp)
This print came out as already seen in the original post.

The second print I did on the same type of paper. Coated also in damp condition right before the exposure, dried with a heatgun. 

The result speaks for itself...

Old coating
PXL_20221124_211925973~2.jpg

Fresh coating
PXL_20221124_211939237~3.jpg

I will not precoat my paper anymore 😉

Best regards
 
Reply 0 0